    Re: drying parameters for technomelt PA 638

    thank you for your feedback, i will check this.

  2. #2
    Join Date
    Jun 2014
    Location
    EU
    Posts
    125

    Re: drying parameters for technomelt PA 638

    Hi,
    Rick is probably right, this seems like process temperature setup in the IM - not drying.

  3. #3
    Join Date
    Dec 2012
    Location
    Serbia
    Posts
    107

    Re: drying parameters for technomelt PA 638

    Hi,

    On Technomelt 678 im using 30C for 4h, and that solved this problem for me. On datasheet is saying that drying is not required but without, surface of parts are like moon surface because of bubbles.

  4. #4
    Join Date
    Oct 2020
    Posts
    20

    Re: drying parameters for technomelt PA 638

    Nemanja Thank you for your feedback, I used the exact parameters you mentioned, then the problem was solved.